Anodizing Dimensional Change: Quote-Stage Fit Guide

Published 2026-11-23 · Tolerances

Anodizing dimensional change on black anodized CNC aluminum parts
Machined aluminum components where coating build is included in the final fit.

Anodizing dimensional change is approximately half the coating thickness on every coated surface. A 15 µm Type II film grows a flat face about 7.5 µm, increases a shaft diameter about 15 µm, and closes a through-bore about 15 µm. Machine those allowances before finishing, or mask the critical feature.

I’m Ashkan, a CNC engineer at CNC Instant Quote. The quote-stage decision is whether a dimension applies before anodize or after anodize. Leaving that unclear can turn a shaft and bushing that both pass inspection into an interference fit. That is one of the CNC Machining Design Mistakes Cost You More Than You Think.

Anodizing dimensional change features on black anodized housings, aluminum brackets, bores, fins, and mounting parts
Bores, shafts, threads, and mating faces need separate coating decisions.

How much does anodizing dimensional change move each feature?

MIL-PRF-8625F with Amendment 2, section 6.10.1, gives the planning rule: an applied coating increases a dimension by approximately one-half of its thickness on each coated surface. Standard Machine’s example is direct— a 0.004-inch coating requires approximately 0.002-inch pre-machining allowance per surface.

Ruijin’s 15 µm Type II example shows how the rule changes by feature. A flat face grows about 7.5 µm. A shaft diameter grows about 15 µm. A through-bore closes about 15 µm. With a 50 µm Type III film, those planning values become about 25 µm, 50 µm, and 50 µm.

Feature15 µm Type II50 µm Type IIIUse when
Single flat faceGrows about 7.5 µmGrows about 25 µmMating face or datum
External shaft diameterGrows about 15 µmGrows about 50 µmBushing, bearing, or pin fit
Through-bore diameterCloses about 15 µmCloses about 50 µmGauge, shaft, or clearance fit
60-degree thread pitch diameterGrows about 30 µmGrows about 100 µmFastener or mating nut

The ratio is similar between Type II and Type III. The risk is not. A 50 µm hard anodize dimensional change can consume most of a 0.10 mm fit allowance, especially on small shafts, bores, and tapped holes.

See also: cnc online quote

Which dimensions should be machined before anodize?

Use “final size after anodize” for the dimensions that must work in assembly. Use “machined size” for dimensions inspected before finishing. A drawing that gives only a nominal size does not tell the machinist whether to cut oversize, undersize, mask, or finish after coating.

For an external shaft, machine the diameter undersize by the expected growth. For a bore, machine it oversize by the expected closure, or keep it uncoated. For a sealing face or datum, specify whether the surface remains coated and where rack contact is allowed.

Why can a 60-degree thread bind when the major diameter looks acceptable?

A 60-degree thread can fail on pitch diameter before the major diameter fails inspection. Thread geometry magnifies radial coating build: pitch diameter changes by roughly four times the per-surface growth, while major and minor diameters change by about twice that growth.

A 50 µm Type III film can increase an external-thread pitch diameter about 100 µm. The crest may look acceptable with calipers, while a mating nut or thread gauge stops halfway down. The practical choices are an adjusted thread size, masking, or post-anodize chasing treated as rework.

What should an anodize note include at quote stage?

A quote-ready anodize note names the type, thickness, alloy, masking, rack contact, and inspection condition. It also marks which dimensions apply before finishing and which apply after finishing. At CNC Instant Quote, we record Type II versus Type III, coating thickness, alloy, masking, and the required size condition from the CAD and drawing.

  1. Name Type II or Type III and the thickness. Failure mode: a Type III coating is quoted against a Type II allowance.
  2. List the alloy and temper, such as 6061-T6 or 7075-T6. Failure mode: coating build and fit behavior are judged against the wrong material.
  3. Mark bores, shafts, threads, seals, and datums that must work after finishing. Failure mode: pre-finish inspection passes but assembly fails.
  4. Show masking, plugging, or permitted rack-contact areas. Failure mode: an uncoated patch lands on a visible or functional surface.
  5. Label every critical dimension as machined size or final size after anodize. Failure mode: machining and inspection use different conditions.

If material selection is still open, compare the process implications with the cnc machining milling guidance before you lock the finish. If masking or extra inspection adds setup work, include it in the quote; related cost drivers are covered in CNC Machining Tariffs 2026: Why Your Quote Costs More.

Your CAD geometry also determines whether the part belongs on a mill, router, or turning center. Review routing milling when broad profiles and rotational features share one part.

See also: CNC Online Quote Threads: Avoid Clarifications

How do you verify a post-anodize fit?

Verify the post-anodize fit with a first article, witness coupon, or functional mating inspection. The half-thickness rule is the design baseline, but tight Type II dimensions deserve measured evidence because actual build can run lighter than the estimate.

Ruijin reports an anonymized composite example involving a 6061-T6, Ø6 mm g6 shaft and a customer-supplied Ø6 H7 brass bushing. Before coating, the shaft measured 0.004 to 0.012 mm below nominal. After a 15 µm Type II coating, it measured 0.003 to 0.011 mm over nominal. The resulting clearance range became approximately −11 to +9 µm, so the knob interfered even though both parts passed pre-finish inspection.

For production, measure the same alloy and temper before and after coating. Record the shaft or bore size, coating thickness, and functional gauge result. A coupon from the same lot can establish actual build before hundreds of parts receive the finish.

End mill cutting an aluminum block before anodizing allowance is applied
The final fit is controlled in the machining program before the coating is applied.

FAQ: anodizing dimensional change and fit

Is Type III always twice the dimensional risk of Type II?

No. The half-thickness rule is the same. Type III is usually thicker, so its absolute movement is larger. A 50 µm Type III film creates about 25 µm growth per coated surface, compared with about 7.5 µm for a 15 µm Type II film.

Should threads be masked before anodizing?

Mask threads when the final fit cannot tolerate pitch-diameter growth or when the bare thread must remain functional. Otherwise, specify an adjusted thread size before coating and verify it with the mating fastener or functional gauge.

Can masking remove all dimensional change?

Masking prevents coating growth on the protected feature, but it adds plugs, fixtures, labor, and rack-mark decisions. Specify the masked area at quote stage rather than treating it as an inspection correction.

Plan the fit before you upload CAD

Anodizing dimensional change belongs in the machining plan, not only the finishing note. Upload the STEP file with the coating type, thickness, alloy, masking, and final-size requirements. CNC Instant Quote supports CNC milling and turning in aluminum, copper, brass, steel, and plastics. Get your cnc machining service quote with the fit risks identified before production starts. →

#Aluminum Machining #CNC Machining Guides #Design For Manufacturing #Engineering Review